Sofab Inks' Tinfab modules outperform fullerene-based controls in new 85/85 damp-heat stability and fracture energy tests

US-based Sofab Inks has shared new stability data for Tinfab, its tin-oxide nanoparticle electron transport layer (ETL) ink. The results come from 85°C / 85% relative humidity (85/85) damp-heat testing of 30 × 30 cm P-I-N perovskite solar modules. In both data sets, the fullerene-free Tinfab modules kept more of their starting efficiency than fullerene-based reference modules over roughly 500 hours.

Damp heat test (85C/85RH) of 30x30 cm modules over 504 hours: C60 control retains 91.74%, 82.82% and 75.65% at 168, 336 and 504 hours, while two Tinfab modules retain 106.12%/95.93%/96.16% and 99.59%/93.98%/89.85%

Sofab Inks collaborated with Alpha Precision Systems (APS) to perform these tests and fabricate the new sample modules. APS is a U.S.-based provider of slot-die coating systems, vacuum-drying systems, and turnkey solutions for thin-film manufacturing. Through its affiliated companies, APS also offers module prototyping services.

 

In the first comparison, a module built with Tinfab and an ALD-deposited ETL retained 87.0% of its initial efficiency after 504 hours of damp heat, compared to 74.4% for an APS fullerene standard module. The Tinfab module's efficiency rose slightly during the first 168 hours, and Sofab says Tinfab's lead grew steadily across the test period rather than narrowing (data through July 16, 2026).

A second set of 30 × 30 cm modules showed a similar trend. The C60 control module dropped to 91.74% of its initial efficiency at 168 hours, 82.82% at 336 hours and 75.65% at 504 hours. Two Tinfab modules performed better: one stood at 106.12%, 95.93% and 96.16% at the same checkpoints, and the other at 99.59%, 93.98% and 89.85%.

The new results build on the case Sofab has been making for replacing C60, the default electron transport material in high-efficiency p-i-n perovskite devices. Sofab sees the fullerene layer as a major source of voltage loss and a mechanical weak point where fielded modules tend to delaminate. Testing at Arizona State University’s Rolston Lab, which studies the connection between module stability and mechanical stress, found that Tinfab increased fracture energy roughly five-fold compared to fullerene-based layers.

Fracture energy Gc measured at ASU: C60 about 0.35 J/m2, NDI-C60 about 1.27, C60 with ionic salt about 1.43, and Sofab Tinfab with ALD about 2.8 J/m2

Sofab Inks and Alpha Precision Systems previously reported a 22.2% efficient fullerene-free 30 × 30 cm module made on a slot-die coating platform, and in that program one Tinfab module retained 96% of its initial efficiency after 650 hours of 85/85 testing. Sofab has recently completed a $6 million seed round to support its scale-up toward full-size commercial modules.

Posted: Sep 19,2026 by Perovskite-Inf…