Swapping tin oxide for aluminum oxide enables perovskite tandem cells hit 26.9% efficiency

Researchers at the University of Stuttgart, Forschungszentrum Jülich, INL - International Iberian Nanotechnology Laboratory, and 

Solarlab Aiko Europe have developed an ultrathin aluminum oxide (AlOₓ) buffer layer that protects perovskite solar cells from sputter damage during deposition of a transparent front electrode, while cutting material use and processing time compared with the industry-standard buffer layer.

 

In semi-transparent perovskite cells and perovskite-silicon tandem cells, a transparent conductive oxide front electrode is sputtered onto the device using a relatively aggressive process that damages the layers just beneath the surface. Buffer layers absorb that damage before it reaches the perovskite and its adjacent electron transport layer, most commonly a 10-20 nm-thick layer of tin oxide (SnOₓ) deposited by atomic layer deposition (ALD) on top of the C₆₀ electron transport layer. But ALD growth of SnOₓ on C₆₀ tends to proceed in an island-like pattern rather than a smooth layer, leaving pinholes that require the buffer to be made thicker than would otherwise be needed. The team instead deposited a 3-5 nm-thick layer of aluminum oxide by ALD at a lower temperature of 75°C. Unlike the tin precursor used for SnOₓ, the trimethylaluminum precursor used to grow AlOₓ does not chemically attack the perovskite and instead passivates its surface, letting the layer grow more uniformly and with better coverage despite being far thinner. 

 

Electron microscopy and X-ray photoelectron spectroscopy confirmed that a 3 nm AlOₓ layer covers the underlying C₆₀/perovskite stack more completely than a 20 nm SnOₓ layer, and grazing-incidence X-ray diffraction showed the thin AlOₓ layer kept the perovskite's crystal structure undamaged through ITO sputtering - matching the protection offered by a SnOₓ layer seven times thicker.

Because aluminum oxide is a wide-bandgap insulator, a layer thick enough to block sputter damage would normally also block charge extraction. The team found their ALD-grown AlOₓ forms with a bandgap of 3.9 eV, well below the 6.9 eV reported for stoichiometric aluminum oxide, with defect-related electronic states within that gap that support charge transport via hopping. Devices with a 3 nm AlOₓ buffer showed higher conductivity (4.78 × 10⁻⁵ S/m) than those with a 20 nm SnOₓ buffer (1.21 × 10⁻⁵ S/m) and displayed ohmic rather than diode-like current-voltage behavior, indicating more efficient charge transfer despite AlOₓ's larger conduction-band offset with the C₆₀ layer.

Semi-transparent devices with the 3 nm AlOₓ buffer reached open-circuit voltages of 1.14 V and fill factors up to 82%, closely matching devices built with a 20 nm SnOₓ buffer (1.16 V, fill factor above 75%), and both buffer types exceeded 17% power conversion efficiency. A thinner 1.5 nm AlOₓ layer proved insufficient to prevent sputter damage, while layers thicker than 8 nm began to block charge extraction and reduce fill factor. Integrated into a two-terminal monolithic perovskite-silicon tandem cell, the 3 nm AlOₓ buffer delivered a stabilized efficiency of 26.9% with a 77% fill factor and negligible hysteresis, compared with a SnOₓ-buffered device that ranged between 26.6% and 27.2% depending on scan direction and showed a 3.76% hysteresis index.

The AlOₓ-buffered tandem cells also proved more robust under stress testing: unencapsulated devices retained 99% of their initial efficiency after 1,000 seconds at maximum power point, compared with 93% for SnOₓ-buffered devices; showed no efficiency loss after 70 minutes at 65°C, where SnOₓ-buffered cells lost 4%; and degraded only about 2% after 4 hours at 85°C, versus an 8% drop for SnOₓ-buffered devices. AlOₓ-buffered cells also resisted moisture-driven degradation better than their SnOₓ-buffered counterparts in a water-droplet test.

The authors noted that a 3 nm AlOₓ layer was thin enough to still allow efficient charge extraction across the C₆₀/ITO interface, despite aluminum oxide's insulating nature - a result they say was unexpected given how effectively the same thin layer blocked sputter damage. They conclude that while ALD is often seen as too slow a process for large-scale tandem manufacturing, the reduced material consumption and simpler deposition of an ultrathin AlOₓ buffer point toward a way to ease that bottleneck.

Posted: Sep 23,2026 by Roni Peleg